1. SCOPE
This specification covers the requirements for one type of flexible, electrical insulating, extruded tubing
whose diameter will reduce to a p r edetermined size upon the application of heat in excess of 121°C (250°F).
1.1 FORM
The tubing shall b e flame retarded an d shall be black with a th ermoplastic h ot melt adhesive lining, unless
otherwise specified.
2. APPLICABLE DOCUMENTS
This specification takes precedence over documents referenced herein. Unless otherwise specified, the latest
issue of referenced documents applies. The following documents form a part of this specification to the
extent specified herein.
2.1 GOVERNMENT-FURNISHED DOCUMENTS
Military Documents
MIL-T-83133 JP-8 turbine fuel (NATO type F-34)
MIL-PRF-5606 Hydraulic Fluid, Petroleum Base, Aircraft, Missile and Ordnance
Skydrol 500B Aviation Hydraulic Fluid
Av Gas (100/130) Aviation Gasoline
A-A -694 5% Na Cl solution
MIL-STD-104 Limits for Electrical Insulation Color
2.2 OTHER PUBLICATIONS
American Society for Testing and Materials (ASTM)D 2671Standard Methods of Testing Heat-Shrinkable
Tubing for Electrical Use
(Copies of ASTM publications may be obtained from the American Society for Testing and Materials, 1916
Race Street, Philadelphia, Pennsylvania 19103.)
ISO 846 Plastics-Evaluation of the action of microorganisms
Page 2 SPECIFICATION RW-3032 ISSUE 1
If this document is printed it becomes uncontrolled. Check for the latest revision.
3. REQUIREMENTS
3.1 MATERIALS
The tubing shall be fabricated from thermally stabilized, modified polyolefin and shall be crosslinked by
irradiation. It shall be homogeneous and essentially free from flaws, defects, pinholes, bubbles, seams,
cracks, and inclusions. It shall have an interior coating of thermoplastic adhesive.
3.2 PROPERTIES
The tubing shall meet the requirements of Table 3.
4. QUALITY ASSURANCE PROVISIONS
4.1 CLASSIFICATION OF TESTS
4.1.1 Qualification Tests
Qualification tests are those performed on tubing submitted for qualification as a satisfactory product and
shall consist of all tests listed in this specification.
4.1.2 Acceptance Tests
Acceptance tests are those performed on tubing submitted for acceptance under contract. Acceptance tests
shall be: dimensions, longitudinal change, tensile strength, ultimate elongation, secant modulus, flammability
(jacket only), and heat shock. Statistical process control data may be used to demonstrate conformance for
dimensions.
4.2 SAMPLING INSTRUCTIONS
4.2.1 Qualification Test Samples
Qualification test samples shall cons ist of 50 feet (15 m) of black tubing. Qualification of any size within
each size range specified below shall qualify all sizes within that size range.
Range of Sizes
1/8 through ¼
3/8 through 1
1-1/2 through 4
4.2.2 Acceptance Test Sample
Acceptance test samples shall consist of not less than 16 feet (5 m) of tubing selected at random from each
compound batch or the first sleeving production lot of the batch compound. Physical property tests
performed at this time qualify subsequent sleeving lots produced from the same compound batch.
4.3 TEST PROCEDURES
Unless otherwise specified, perform tests on specimens which have been fully recovered by conditioning for
5 minutes in a 150 ± 5°C (302 ± 9°F) oven. Condition the test specimens (and measurement gauges, when
applicable) for 3 hours at 23 ± 3°C (73 ± 5°F) and 50 ± 5 percent relative humidity prior to all testing. Use
mechanical convection type ovens in which air passes the specimens at a velocity of 100 to 200 feet (30 to 60
m) per minute.
SPECIFICATION RW-3032 ISSUE 1 Page 3
If this document is printed it becomes uncontrolled. Check for the latest revision.
4.3.1 Dimensions and Longitudinal Change
Measure three 6-inch (150 mm) specimens of tubing, as supplied, for length ± 1/32 inch
(± 1 mm), and inside diameter in accordance with ASTM D 2671. Condition the specimens for 5 minutes in
a 150 ± 5°C (302 ± 9°F) oven, cool to 23 ± 3°C (73 ± 5°F) and then remeasure. Prior to and after
conditioning, the dimensions of the tubing shall be in accordance with Table 1 and the longitudinal change
shall be in accordance with Table 3. Dimensions of adhesive thickness shall be taken from specimens which
have been hung vertically in the oven during recovery. The adhesive thickness shall be the average
determined by measuring a cross section taken 1 inch from each end of the suspended specimen. Care should
be taken not to overheat the adhesive so that it drips or flows from the tubing.
Calculate the longitu dinal change as follows:
C = L1 - L0
L0 x 100
Where: C = Longitudinal Change [Percent]
L
0 = Length Before Conditioning [Inches (mm)]
L
1 = Length After Conditioning [Inches (mm)]
4.3.2 Tensile Strength and Ultimate Elongation
Determine the tensile strength and ultimate elongation of the tubing in accordance with ASTM D 2671 using
1-inch (25-mm) bench marks, a 1-inch (25-mm) initial jaw separation, an d jaw separation speed of 20 ± 2
inches (500 ± 50 mm) per minute.
4.4 REJECTION AND RETEST
Failure of any sample of tubing to conform to any one of the requirements of this specification shall be cause
for rejection of the lot represented. Tubing which has been rejected may be replaced or reworked to correct
the defects and resubmitted for acceptance. Before resubmitting, full particulars concerning previous
rejection and action taken to correct the defects shall be furnished to th e inspector.
5. PREPARATION FOR DELIVERY
5.1 FORM
The tubing shall be supplied in lengths of 48 +1, -0 inches (1220 +25, -0 mm) unless otherwise specified.
5.2 PACKAGING
Packaging shall be in accordance with good commercial practice.
5.3 MARKING
Each container of tubing shall be permanently and leg ib ly marked with the size, quantity, manufacturer’s
identification, specification number, and lot number.
Page 4 SPECIFICATION RW-3032 ISSUE 1
If this document is printed it becomes uncontrolled. Check for the latest revision.
TABLE 1
Tubing Dimensions
Dimensions -
inches (mm)
Size
Minimum
As Supplied I.D.
Maximum
Recovered I.D.
Nominal
Recovered Wall
With Adhesive
Nominal Recovered
Adhesive Thickness
1/8 .125 (3.17) .062 (1.57) .027 (0.68) .009 (0.23)
3/16 .187 (4.74) .093 (2.36) .028 (0.71) .010 (0.25)
1/4 .250 (6.35) .125 (3.17) .029 (0.74) .005 (0.13)
3/8 .375 (9.50) .187 (4.74) .029 (0.74) .005 (0.13)
1/2 .500 (12.7) .250 (6.35) .030 (0.76) .006 (0.15)
3/4 .750 (19.05) .375 (9.50) .035 (0.89) .006 (0.15)
1 1.00 (25.40) .500 (12.7) .042 (1.06) .008 (0.20)
1-1/2 1.50 (38.10) .750 (19.05) .047 (1.20) .011 (0.28)
2 2.00 (50.80) 1.000 (25.40) .065 (1.65) .022 (0.56)
3 3.00 (76.20) 1.500 (38.10) .065 (1.65) .022 (0.56)
4 4.00 (101.60) 2.000 (50.80) .070 (1.78) .020 (0.51)
TABLE 2
Mandrel Dimensions for Bend Testing
Tubing Size Mandrel Diameter
in.
mm.
1/8” to ¼” inclusive 5/16 7.9
3/8” to ¾” inclusive 1/2 12.7
1” to 4 “ 9/16 14.3
SPECIFICATION RW-3032 ISSUE 1 Page 5
If this document is printed it becomes uncontrolled. Check for the latest revision.
TABLE 3
Requirements
PROPERTY UNIT REQUIREMENT TEST METHOD
PHYSICAL
Dimensions
Inches (mm)
In accordance with
Table 1
Section 4.3.1
ASTM D 2671
Longitudinal Change Percent +1, -5 ASTM D 2671
Tensile Strength psi (MPa) 1500 minimum (10.3) Section 4.3.2
ASTM D 2671
Ultimate Elongation Percent 200 minimum
Secant Modulus (Expanded) psi (MPa) 2.5 x 104 maximum
(172)
ASTM D 882, 2%
strain
Cold Impact
at -55 ± 2°C (-67 ± 4°F) --- No more than 5 of 10
crack ASTM D 746
Proc. A
Heat Shock
4 hours at 250 ± 3°C (482 ± 5°F) --- No dripping, flowing
or cracking of outer
wall
Table 2 mandrels
ASTM D 2671
Heat Resistance
168 hours at 175 ± 2°C (347 ± 4°F)
Followed by test for mandrel bend
--- --- ASTM D 2671
Table 2 mandrels
360 ° bend in 10 ± 2
seconds
Color Stability
48 hours at 175 ± 2°C (347 ± 4°F) --- MIL-STD-104 ASTM D 2671
ELECTRICAL
Dielectric Strength
Volts/mil
(volts/mm)
500 minimum
(19,680) on dual wall
specimen
NOTE 1
ASTM D 2671
Volume Resistivity ohm-cm 1014 minimum on
dual wall specimen
ASTM D 2671
CHEMICAL
Copper Mirror Corrosion 16 hours at 121 ±
2°C (250 ± 4°F)
-
--
No removal of copper
ASTM D 2671
Procedure A
Copper Contact Corrosion
16 hours at 121 ± 2°C (250± 4° F) --- No pitting or
blackening of copper ASTM D 2671
Procedure B
Page 6 SPECIFICATION RW-3032 ISSUE 1
If this document is printed it becomes uncontrolled. Check for the latest revision.
TABLE 3
Requirements
(continued)
PROPERTY UNIT TYPE 1 TYPE 2 TEST METHOD
CHEMICAL (continued)
Flammability (jacket only)
---
Self-
extinguishing
within
1 minute, 25%
maximum flag
burn
---
ASTM D 2671
Procedure B
Water Absorption
24 hours at 23°C (73°F) Percent 0.5 maximum 0.2 maximum ASTM D 2671
Fluid Resistance
24 hours at 23°C (73°F) in:
JP-8 Turbine Fuel (MIL-T-83133)
Skydrol 500B
Hydraulic Fluid (MIL-PRF-5606)
Avaiation Gasoline (100/13 0 )
5% NaCl Water
Followed b y tests fo r:
--- --- --- ASTM D 2671
Dielectric Strength Volts/mil
(volts/mm) 400 minimum
(15,760) 400 minimum
(15, 760)
Tensile Strength psi (MPa) 1000 minimum
(6.9) 1000 minimum
(6.9)
Fungus Resistance
Followed by tests for:
Tensile Strength
Ultimate Elongation
Dielectric Strength
psi (Mpa)
percent
Volts per mil
(volts per mm)
1500 minimum
(10.3)
200 minimum
500 minimum
(19,680)
1500 minimum
(10.3)
200 minimum
500 minimum
(19,680)
ISO 846
Method B
Section 4.3.2
ASTM D 2671
ASTM D 2671
*Trademark of the Monsanto Company
NOTE 1: Recover the specimens on the metal mandrels for 10 minutes, minimum, at 150 ± 3°C (302 ± 5°F) or until the
tubing is completely shrunk on the mandrels.